You are on page 1of 17
EUROPEAN STANDARD FINAL DRAFT NORME EUROPEENNE EN 1168:2005 EUROPAISCHE NORM. prAt hay 2007 1e591.06020;91 10020, English Version Precast concrete products - Hollow core slabs Peau pnt enon. Ole aoe exam rin ‘na aentnet tape nth he Eungn Sed BI E8285 hs Sco at CON prwcutsn anne arse ors CEN marae mots Son anny sod mateo be Gen argue Comes Bae ance xy Se, nga, ay so reat ana ts aa Nay PO a omni Sai Sei Sn Swe ees ee z Managem Carr de Seer. 36-480 Gale EN 4460:2008/prAt:2007 (E) Foreword ‘This docurort (EN 1168200S/prA:2007) hasbeen prepare by Technical Commitee CENITC 228 Precast coreelepodct Ie sacrearat when shelby AFNOR, “This docurent i curt submit tothe Unique Acceptance Proce, ‘This cocunert hes been prepared under 2 mandate gen to CEN by the Euzopeen Commission and the European Free Trade Asscison, and supports essential requrements cf EU Dect). For relationshp wth EU Deeciv(s), se infomnatve Annex ZA, whichis an negra pat ofthis document EN 1168:2008/prA1:2007 (E) 1. Modification to Clause 1 Scope ‘nto 7 sentence ofthe 6 paragraph change "450" it's" 2 Modification to.4.3.1.1. Production tolerances Change the number of he second sutclause numbered 34.1.1" nfo"43.1.12" and he numbering of 3. Modification to 4.2.1.1.2 Tolerances for concrete cover Inpoit43.1.1.2 (now 43.1.1.) node the sentence “The maximum devation fr conte cove shal be ‘Sce-1D man A move stinger llerance canbe declared by tne menufere? 4. Modification to 4.3.1.2.2 Minimum concrete cover and axis distances of Prestressing steel FRepaco” - wen the rain centre to conte stancsofthe strands» 28 omin= 180. hen he nominal cee to ceave stance othe sands «28 om = 280: “"Gnin may be derved by near mterpolatonBeween the vie clsvated Ina) and) 2's the sand ox wi daretr in mimes (nthe case of ferent cetars in a strand.the average ‘ole sha be ued foe Forritbed wes, the concrete cover shal be mereared wth 1 2° a 8) “when te nominal conte to centre stance ofthe sands is 23 2) wen he nominal centre to conve distance of the sands is <2.8 6 n= 28% thor @ is the stand ox wie ameter in mitimetes (in he case of erent carers, th average vale Shab uted or Fos intraciat cate to oente distance, can may be detved by car Inerpolaton between the valves tino in 2) ana, For ibbed wis, he concrete cover shal be incoased by 1 ¢* 5 Modification to 4.3.3.2.1 Resistance to spilting for prestressed hollow core slabs ‘nt le of 4 3.22.1 snd inthe re of he oxt of 43.3.2 1, replace ve tes “pltig” wih "spaling” EN 1168:2006/prAt:2007 (E) 6 Modification to 4.3:3.2.24 General Change the tile"“Ganar” ino "Shee capacity” ‘Ado fouing text ate the tte (beer the exiting statement) “For holomcor sabe without shear riefrcement, he shear estan of he repons cracked by bending ‘halbe calclted using expressions (62a) and (6.0, EN 1952--1 2008 For prestessod single span hotowicue site wiht shear reinforcement, the shear resistance ofthe regions unracted by bending (where the extra! lela sess fe sraler han fg), he sheat ‘esitence shoud be caluaid wth te flowing expression tae = et uaF eeVFea ~F)) ao rere te wot Se no caine SAM Snead] ba} “This expression cha be ape win reference to thecal pons of 2 staph ine f flr ising tom the ‘ce of te support wih an angle = 35" wa eapet oe horizontal si, The etal pots the po on ‘he quoted ne where the res oe exposson of Fag the lowe “The defton of eymtoeis given here below: 0) wa with at he ria point isthe heph of he conde xs 4) fthefet moment othe area above height nd about be conto se 1 tsthe bight of the tia point on the in fre J, the stance ofthe considered pont onthe ie fate fromthe staring panto the vanemiesion eng =) el) she concrete comeressve sve atthe hei y and istance I, 1 tethe number oftandon ayers 4 wthe area ofthe cross-section i) tte presvessng force in he considered tenon at stance The raneet of prestess shal be taken ite secourt secon to 810.22 of EN 1982.1-1:2004 Mey ie bending moment de to the vertical lad, for he epresion the bending mement may be ‘grored Me ‘o) inte concrete shear stesso Yanemiaion of pesress atheight y and datos, AS) tne ee sore thy ‘6x62 actor taking it account the postion fhe considered tendon ayer Gye when vs 7A, m2 0 when 7 70, le the height ofthe postin cf considered tendon tye ‘As an aemstive tothe above expression, he ollowing smpiid expression may be applied Frac 0 Lea? + Bartels 1s se second over tt moment ara (=: ve a) idle te cage of pestennguananison (4 10) 4 is te dre te eno eton fer sat pnt rare gh lp uppers of anemone (eo (8 18) of EN 1921-208) ie the fil conerete compressive sess at he cenidlais is the design vu of terse evens of concrete: reducing ttn reducing tater rela to ranemiasion ath Fer hollow-core sibs deepe’ than 450 rm the shear eng, bah for regions crecked or unracked by bondng hale edocoa by 0,9 wah repectto he equations usted above 7 Modification to 4.3.3.222 Shear capacity - Torsion capacity Change te tin “Shear wi ron capt" 8 Modification to 4.3.3.2.3 Shear capacity of the longitudinal joints ‘Ator"Dhs he sumof be uate! hiekresses of th upse andlonee tage andthe scl ties of he {oyping (00 Fp 4) ee te folowing cortence where he ssid thekness she manatees fhe ‘ogping muled by the ratio between the tense crergi fhe oppng ara the tone senth of te ate EN 1168:2008/prA1:2007 (6) 9 Modification to 4.3.6 Thermal properties Inthe explain of Re change “conta ino"autce” 10 Modification to 6.2.1.1 Procedure In indo change "43.14.22 info“. 3.11 10" and n indent) change" 3.14.26" tora3.3..367. 114 Modification to Annex A- Table AS In tom 1, # column (Pupose) change sear ressanca info "Tab 42 Modification to Annex B - Figure 8.4 Change thefower dimension of Figure Bf) 25 foows 4 | rE [ | (=| Las . a | | Key 4, Large ona mesma agra fe moar thot Figure B.1—Typleal shapes of orginal ont EN 1168:2006iprA4:2007 (©) 48 Modification to Annex C - Figure C4 In Figur C4) and) show to positon of the sd as folows ma + coo CEPT 8) Pint ioad ncerte 6) Pont ad batwoen c)Linearloadin conte) Linear load notin cate ‘corte ad supper Figure C.4— Assumed shape of vertical shear fores in joints 14 Modification to Annex ¢ - Figure C6 In Figure C8 change the ecole 28 flows: [+7 te TS See . f ma POE See Koy 1 racer free pani nas 2 Sanam 3. patios Figure ©. — Reaction force at longitudinal support dve toa pont load at midepan EN 1168:2005/pra1:2007 (€) 118 Modification to Annex E -E.2 Design by calculation Fepiace Expression (2 wih tho flowing 416 Modification to Annex F - F.2.2 Failure typ: In tho 2 expression poche. 117 Modifestion to Annex F -F.2.2 Failure types a Resiac the 9 expression wih: a Baveonles cing the reteronce ‘ix and ps00433224) 418 Modification to Annex F -F.2.2 Failure types a In tls tw Stntion pace I" With lg Bg Wh eg 419 Modification to Annex F -F.3 Shear tension capacity of a hollow core slab with a umber of filed cores. ‘Replace exresson wih be feowing 2 Yaa Ete 20 Modifiestion to Annex J Replace te fest of Anex J wi th fotowing EN 4168:2008)prA4:2007 () Annex J (normative) Full scale test JA General ‘The test laments shal be reprosonative ofthe cross section or produc omy: ol pestressing force for peateesed halon ox of rforsement aroun for eevee haw ote shal bea east he 78% of he fmaxeram scheduled forthe given cos secon 2 Apparatus ‘The esting mechireshallbe at last a clas 3 machine accorang Wo 42 of EN 128804.2000, J Test arrangement Tests salle card ot by the manulactur a testing laboratory onthe ato, Thott shal be pred at a emperatire of °C to 40°C. This temperature shal se recorded In exer to get erence vaties of the svength of the concrete (aect etuctul stength — ene EN e960.2004, 42.22.) cynical cores shal be riled ou f te lament. To obtain hese cores, asad ‘sogientc 200 m5! langthshal be sown out fom tne easing bad, rey adjacent to te test Specmons. This semen shat be coneeved under the some sonston of fhe eo spsemene Shot bles {esing, thre corey sha be dle out ofthe slab segment (oe also Table A3) ars that sengih shal be ‘measured tin 3 days rom tne Ste of the est The aan ofthe tee messized valves gs the ctl Comprescve songth/. Inctoad of ded eve, nordero get reference values of he strength of he conciet, 3 spacmens (cubes cr Cylinders) may be nase sung he fabieaton of fhe let element sro submited to he same heat eaten Uindvecstuctralsengin "see EN 13280-2004, 42.224) The specimens shal be centered under the ‘ro condtore atthe fat element The compressive svengn ofthe epecznan sel be messes wf Stays tom ihe soe Othe fat ne tear othe tes Measured vats Qe he ctl compressNe Seong ‘The same type of test specimens (sed cores or eubesieinder) shal be used atin factory production corto astecs coformity of concrete stengh In smiar way, when the actal tense corereto stength fy Is messued ty spting tone fete (see 812 (8) of 1952-12008), t shal be taken as the mean fhe 3 tests ruled by 0.90, ‘The tos eloment sallbe a fubwidth sab element wih a span of Amor 53x, whichever egg, wih the tolerance of 100 mm Initia ype testing chat be done cote clement wih th same presetsingreinkcement The age the testelaments ehaie et ese 26 aay EN 1168:2008/prA1:2007 (E) ‘The supper hich ste nearest othe oad appleaton point shal be a rllr beara, so that no axial forces. tre generated by oan te clmert lhe support Batwoon the element end he suppet boa oa ‘sous marl such a8 10 ren asonte or neepere of a Bed of moto gypsum shalte applied. Ths ‘malo! hes to compensate forthe unevenness of the element sutace nd a possile caveture ofthe ‘ment inthe transverse drection. he ad shal be apple a the distance fom the rol szpport of 2:5 ‘ware his the fll depth ofthe cross-section, bu no lesser han 600 me wih fe tolerance #25 ym The: ‘topo coats shal be such thatthe suppod reaclon © unformy dstoued over th wath ofthe menbec ‘The oad shall be reduces by 2 tif wansverse steal bea, The sitfrass of is beam shallbe scent to prove nonuniform dtrbuson of te ead ove the with fhe bear. “The denn ofthe steel beam eallbe at eat 150 men, but when using one ack, peerably 250 Diensioe in mites. ©) Ona ine fading 2) Two nes loasing 10 EN 1168:2006ipeAt:2007 (6) ©) Dea of suporin a) ab) JA Loading procedure ‘Tho loa shal be spptad ae repeated loading in 2 cyl, The alts of th oad of he fa yc shall be equal atest 13% wih lrarce oP % and» 7h, of he roqured Sesign imate os. the lat ‘je the lad salbe increased uno the actu uate oad a fre “Te required design ulate ea sha be evatsted using the design model ofr with he design value {or materia proprts, nominal devenlons and wih egarto he mos nfavurable are made “The speedo th ago the etemert shal rt excons the flowing mas: ~ forthenistcyce — wo steps t equal amit none minute each and subseavent withdrawal fhe fad — forthe seconaeyce — tt sep up to 50% of be cleat uate ead none minut: — second op upto 75 % of the utmate ead none minute —subsequert crease ofthe oad with speed not exceeing 10% of he caleisted timate fad par The caleusted ubmte ead Fy, shal be evaluated using the design made for fate, wth the actust strength parameter of see, wih the actual srongth parameters of concrete derives om ke compeest ve ‘Stength such as rasinedin 3. aking due ™g" 0nd ye = 100, waht acta enensions and wih ‘gard tote rest snfaveurabl are mode, Istad of derived rom canpressveerengh tensile strength toner may bemeasured by tests ese 3) “The actual ulate load corasponding to the fare ofthe tet element shal be rected together wth te Indication ofthe fare mee (cea onsen, shear Neue, anchorage, eackng mame). 1“ EN 4468:2005/prA:2007 (€) J Interpretation of results ‘The falure mode cbserved in he et should correspond othe model assumesin cael. “The resus o he test shat be erected agains the escusted uta load Fa NOTE. The cesgn modelo thea ue is ereenad by Equations (2) (6.4 of EN 19521-12004, vere these compat month sumed ce go fe scares sengih a's aed pose ag Saka tare soon may Oe meas ety Dy et Gees By Ee canons of Tate 3 of EM TZ" 204 (rer 8 paced by ond gh mln by teugh elton cleus 12 Ite, +810) er concae classes > CSO 8 fan ‘The sess ci de to presvocs shall be cacusted, wt = 1, taking ito account tho presesing losses developed at be tet time anda near increase over te ranemisson lang ly at dened by expression (8.16) of EN 19021-12004. The fret uncreched socton to ba checked fr fare i placed at 2 fom te ‘topot (Selective dep. The fst poesbleeacton cracked by Bencing moment e paced rm te. Epport Tho cracking bendtg, memont i compulod wih fq. For tose eatclabons the res of EN 1992112004 ae apples ‘The design model elabity is cnfimed de olowng requirements se fulles Fd! Fasc? 098 foreach test ‘Avero00 (Fa! Fe) 2100 forthe mesn ofthe tes tests Frau: % the cakulated utinate load conespending te he flre mode cbserved foreach nual ect semen Fag 00 octal ultimate led foreach ndhidul est eement ‘Average (Fad Foxe) 'S the mesn valve of the tee ratios betwoon each scl! Utimate lad and the coresponding xpacied ulimot ad 1 te tet resus do not comply wih the two requremens stove, one ofthe flowing actos shall be Una ‘= kmprove production (machinery andor conceta mi) end test aga vee new es loners —sustne design mode fee design ofthe product 12 EN 4468:2008/prA4:2007 (E) JS Test report “The test rport sal cide = te ienfeaton ofthe et element — the dat of manufactur or any ote coe; the date nd ple tsi: — tre laneratry an tn prton in charge of testing — alin scl peperes of meter used forthe test element: = tetest metho, — tne moasuing exapment wed — he tomperture tine ecaton testing: = theatre oad ae: = thetaiure medeincusng writen cession ane photos: — any observation regarding the tee and any ordre ed (racks, te) — 2 declaration that the tes has been cared out in campfance wih th stander, pus detats of ny ‘snencnert mace” 8 Carla Ramalhoto De: NIP -Assoiagso Nac. do ln. de Prelabreaco em Beté [aipb@netcabo ot) Enviado: {ergafra, 2 ce Outro do 2007 16:06 Para 125: SECic PREBETAO (Jodo Portela. ARISTIDES DE SOUSA; 68 - RUBETAO (Hugo Novos Anti 47 ARTEBEL (Sve Neves) ce: Carls Remainte ‘esunto: FIVSEN TTEBPrat -Furber editor eror ens kone Mensagem orignal De Prot. landomenica Teno maltetoniclo@stpoin) nada treater, 2 de Out de 2007 15.08 Pra: svelexdberkne.no; Me Amada; cn constuccon@aenor-es; david. appleton@hanson biz. ‘bovermelster@lipran de tbo or; bennenkcors(@wortorine.n aaririsvaclo@hermpree2.om; Sahoston bemaai@recior fr: cateborfani@atoe it boscoc@pelto ka chefosbion@oara. com’ Jcobecerrumpaslo doe cuche@skynet.e:ed@febo be. sce boo @icluse jw @ayere Por@gruppocenvonorat: hah og try sliotigmaororocasl. com; MG. Fiuereredo,) Archer de Samnisracio@hormiprose com: gsper_a@lbero I; carve glmarn@ecter alos ara a jan {aude hesng@inorf teune hetanen@@betn| com; uegerace com m hurez@eer com ose lelo@evival pt B56 Becrum@BOzerentdo: rc. Mingeeo, face consting vanadoo acto napos@oatio “andro onderbeke@probeten be; Palteon M@rabya9 =p oYGNDI MT, quasi@ls hamburg. ‘oncheti@osseveon ty eller wot opbeturtode athe sheer no. cart iichelourter@eram bctogno fr mv@valcate com: v vime@sluk ce 1. Waaven aly wah Mubecske@veeb co a hlayor@buntemel com, marca menegclogunromet. mats bors@oetongranundustin se Marta Perelo Redondo: a@ibm of ulthonbergiela com, michal netrebe@eder a: wolgangdiece ‘hard siverur@isespfrmicl@ing uno jen horcamane@Dprabeton be: gsagei@hetet ni welingg@eten nk Imeoncecaog@mal lsepac pt ane@andece or joachim Kapacek Qn de, lderwaldgzap" gmbh de {aco vandonbroek neni gosta nase @srangbelog.c, rane ctmar@europcles com ‘S.ovind olesend@mal dk st maas @ochobel comb barnoudeers com, lI Ce ‘oman browniitshprecattorg smannicoferbgtoibsu de [Retunio: EN 68ipeAt Furor odors! oor Fotowing the rca ecaved tom the German coleague Misch, inform you tat the equation for sigma-cp in ‘commont 6 of UAPT for Hallow core elements, presely unde formal vote, ol caret, You can finite correct feuaton inthe attaches Pesse pont out his esto eorin your vot, Best regards ‘Gancomenico Tonioto This message has been scanned fr veuses and dangerous content by MaiScanne, andi (etlved by ea, EN 1168:2005/prA1:2007 6 Modifikation to 4,3.3.2.2.1 = lbw Scly) de teas? + op (vite ~ Fop(0)} 1) +Cpyiy)} $PA0x)} sly) should be changed into: caw E En 46Q: 2008 / pe Aa. Zor? FF Wor fukn be Awan F_F3 Shen Gros oprcty of = loll ce ‘The correct equation is IAS ity eden of PLE Cons Van = Vide * 2/8 m bed fa

You might also like