HEMPEL A/S
Customer:
Project:
Area:
Area size:
1 sqm
System A (Non insulated) Carbon steel piping,equipment and structural steel, operating temperature up to 120C Substrate Carbon Steel
Surface preparation:
Minimum secondary surface preparation mechanical cleaning to St 3 according to ISO
8501-1:2007, apart from cleaning for surface contamination SSPC- SP1.
Product name
Colour
Film thickness
(micron)
Wet
Dry
Shade no.
Treated area
%
Red
Grey
To Be Advised
Total d.f.t.
Hrs=Hour(s)
50630
12130
T.B.A
Mth=Month(s)
100
150
50
Theoretical spreading
rate
75
125
40
240
(sqm/ltr)
Application methods
Roller
Brush
Spray
10.7
6.4
16.8
Recommended
Nozzle
Nozzle
orifice
pressure
(X)
X
.017"-.023" 250 bar
(X)
X
.017"-.023" 250 bar
X
X
X
.017"-.021" 175 bar
X: Recommended (X): Possible
N/R=Not Recommended
D.F.T.
Quality no
45881
45881
(micron)
Recoated with
quality no
Min.
40C
75
125
45881
55610
115 Min
3 Hrs
30C
Max.
Ext
36 Hrs
Min.
3 Hrs
5 Hrs
20C
Max.
Ext
54 Hrs
Min.
3 Hrs
6 Hrs
10C
Max.
Ext
72 Hrs
Shirish Khare
Sales
1
Quality Code:
Environment :
Severe
Min.
N/R
N/R
0C
Max.
N/R
N/R
Min.
N/R
N/R
-10C
Max.
N/R
N/R
Min.
N/R
N/R
Max.
N/R
N/R
Specification sheet
HEMPEL A/S
Customer:
Project:
Area:
Area size:
1 sqm
System A (Non insulated) Carbon steel piping,equipment and structural steel, operating temperature up to 120C Substrate Carbon Steel
Remarks:
Normal good painting practice must be followed throughout the entire painting procedure.
Product information:
Shade no.
HEMPADUR MASTIC 45881
50630
HEMPADUR MASTIC (MIO )Version 45881 12130
HEMPATHANE HS 55610
T.B.A
Volume
solids %
Curing
agent
80
80
67
95881
95881
97050
Mixing ratio
volume
3:1
3:1
7:1
Pot life
Dry to touch
20C
1 h 30 min
1 h 30 min
2h
20C
3h
3h
5h
Flash
point
C
39
39
31
Thinner
08450
08450
08080
Application restrictions
Min. Temp. Max. RH%
C
15
15
-10
85
The data, specifications, directions and recommendations (hereinafter "Information") given in this painting specification are based upon test results obtained under controlled or specifically defined conditions and said Information is correct to the
best of our knowledge. The User must satisfy itself that it is appropriate to use the Product in accordance with the Information in the actual conditions under which the Product is intended to be used, and the Manufacturer and Seller do not
guarantee the accuracy, completeness or appropriateness of the Information when the Product is used in those conditions. The provisions regarding Hempels liability in its applicable conditions for sale, delivery and service shall apply to any and
all claims arising out of or in connection with the use of the products recommended above, overleaf or otherwise.
Hempel's PreSale System 2.6.17 (Build 900)
User name:
Printed at:
16.02.2015 11:01 Department name:
Created/Last modified:
16.02.2015 10:40 AESHK0084N Page:
Shirish Khare
Sales
2
Quality Code:
Environment :
Severe
Specification sheet
HEMPEL A/S
Customer:
Project:
Area:
Area size:
1 sqm
System A (Insulated) Carbon steel piping,equipment and structural steel, operating temperature up to 120C Substrate Carbon Steel
Surface preparation:
Minimum secondary surface preparation mechanical cleaning to St 3 according to ISO
8501-1:2007, apart from cleaning for surface contamination SSPC-SP1.
Colour
Film thickness
(micron)
Wet
Dry
Shade no.
Treated area
%
Red
Grey
Total d.f.t.
Hrs=Hour(s)
50630
12130
Mth=Month(s)
100
150
Theoretical spreading
rate
(sqm/ltr)
75
125
200
Application methods
Roller
Brush
Spray
10.7
6.4
Recommended
Nozzle
Nozzle
orifice
pressure
(X)
X
.017"-.023" 250 bar
(X)
X
.017"-.023" 250 bar
X: Recommended (X): Possible
N/R=Not Recommended
D.F.T.
Quality no
45881
(micron)
Recoated with
quality no
Min.
40C
75
45881
115 Min
30C
Max.
Ext
Min.
3 Hrs
20C
Max.
Ext
Min.
10C
Max.
3 Hrs
Ext
Shirish Khare
Sales
3
Quality Code:
Environment :
Severe
Min.
N/R
0C
Max.
N/R
Min.
N/R
-10C
Max.
N/R
Min.
N/R
Max.
N/R
Specification sheet
HEMPEL A/S
Customer:
Project:
Area:
Area size:
1 sqm
System A (Insulated) Carbon steel piping,equipment and structural steel, operating temperature up to 120C Substrate Carbon Steel
Remarks:
Normal good painting practice must be followed throughout the entire painting procedure.
Product information:
Shade no.
HEMPADUR MASTIC 45881
50630
HEMPADUR MASTIC (MIO )Version 45881 12130
Volume
solids %
Curing
agent
80
80
95881
95881
Mixing ratio
volume
3:1
3:1
Pot life
Dry to touch
20C
1 h 30 min
1 h 30 min
20C
3h
3h
Flash
point
C
39
39
Thinner
08450
08450
Application restrictions
Min. Temp. Max. RH%
C
15
15
The data, specifications, directions and recommendations (hereinafter "Information") given in this painting specification are based upon test results obtained under controlled or specifically defined conditions and said Information is correct to the
best of our knowledge. The User must satisfy itself that it is appropriate to use the Product in accordance with the Information in the actual conditions under which the Product is intended to be used, and the Manufacturer and Seller do not
guarantee the accuracy, completeness or appropriateness of the Information when the Product is used in those conditions. The provisions regarding Hempels liability in its applicable conditions for sale, delivery and service shall apply to any and
all claims arising out of or in connection with the use of the products recommended above, overleaf or otherwise.
Hempel's PreSale System 2.6.17 (Build 900)
User name:
Printed at:
16.02.2015 11:01 Department name:
Created/Last modified:
16.02.2015 10:40 AESHK0084N Page:
Shirish Khare
Sales
4
Quality Code:
Environment :
Severe
Specification sheet
HEMPEL A/S
Customer:
Project:
Area:
Area size:
1 sqm
System B (Non insulated) Stainless steel piping and equipment , operating temperature up to 120C ,Substrate Stainless steel
Surface preparation:
Oil and grease etc. to be removed by emulsion cleaning. Salts and other contamination to
be removed by high pressure fresh water hosing. Entire area to be roughened to create a
uniform flat finish prior to application of the specified painting system. In severe cases,
abrasive sweep blasting to a uniform flat finish with a dense surface profile may be
necessary. The abrasives used must be non-metallic and metal free. Depending on local
conditions, mechanical cleaning (avoid polishing) may be used.
Colour
Film thickness
(micron)
Wet
Dry
Shade no.
Treated area
%
Red
To Be Advised
To Be Advised
Total d.f.t.
Hrs=Hour(s)
50630
T.B.A
T.B.A
Mth=Month(s)
150
50
50
Theoretical spreading
rate
125
40
40
205
(sqm/ltr)
Application methods
Roller
Brush
Spray
6.4
16.8
16.8
Recommended
Nozzle
Nozzle
orifice
pressure
(X)
X
.017"-.023" 250 bar
X
X
X
.017"-.021" 175 bar
X
X
X
.017"-.021" 175 bar
X: Recommended (X): Possible
N/R=Not Recommended
D.F.T.
Quality no
45881
55610
(micron)
Recoated with
quality no
125
40
55610
55610
40C
30C
20C
Min.
Max.
Min.
Max.
3 Hrs
35 Min
36 Hrs
None
5 Hrs
65 Min
54 Hrs
None
Min.
6 Hrs
2 Hrs
10C
Max.
72 Hrs
None
Shirish Khare
Sales
5
Quality Code:
Environment :
Severe
Min.
N/R
3 Hrs
0C
Max.
N/R
None
Min.
N/R
6 Hrs
-10C
Max.
N/R
None
Min.
N/R
10 Hrs
Max.
N/R
None
Specification sheet
HEMPEL A/S
Customer:
Project:
Area:
Area size:
1 sqm
System B (Non insulated) Stainless steel piping and equipment , operating temperature up to 120C ,Substrate Stainless steel
Remarks:
Normal good painting practice must be followed throughout the entire painting procedure.
Product information:
Shade no.
50630
T.B.A
T.B.A
Volume
solids %
Curing
agent
80
67
67
95881
97050
97050
Mixing ratio
volume
3:1
7:1
7:1
Pot life
Dry to touch
20C
1 h 30 min
2h
2h
20C
3h
5h
5h
Flash
point
C
39
31
31
Thinner
08450
08080
08080
Application restrictions
Min. Temp. Max. RH%
C
15
-10
85
-10
85
The data, specifications, directions and recommendations (hereinafter "Information") given in this painting specification are based upon test results obtained under controlled or specifically defined conditions and said Information is correct to the
best of our knowledge. The User must satisfy itself that it is appropriate to use the Product in accordance with the Information in the actual conditions under which the Product is intended to be used, and the Manufacturer and Seller do not
guarantee the accuracy, completeness or appropriateness of the Information when the Product is used in those conditions. The provisions regarding Hempels liability in its applicable conditions for sale, delivery and service shall apply to any and
all claims arising out of or in connection with the use of the products recommended above, overleaf or otherwise.
Hempel's PreSale System 2.6.17 (Build 900)
User name:
Printed at:
16.02.2015 11:01 Department name:
Created/Last modified:
16.02.2015 10:40 AESHK0084N Page:
Shirish Khare
Sales
6
Quality Code:
Environment :
Severe
Specification sheet
HEMPEL A/S
Customer:
Project:
Area:
Area size:
1 sqm
System B (Insulated) Stainless steel piping and equipment , operating temperature up to 120C ,Substrate Stainless steel
Surface preparation:
Oil and grease etc. to be removed by emulsion cleaning. Salts and other contamination to
be removed by high pressure fresh water hosing. Entire area to be roughened to create a
uniform flat finish prior to application of the specified painting system. In severe cases,
abrasive sweep blasting to a uniform flat finish with a dense surface profile may be
necessary. The abrasives used must be non-metallic and metal free. Depending on local
conditions, mechanical cleaning (avoid polishing) may be used.
Treated area
%
Shade no.
Colour
Red
Total d.f.t.
50630
Film thickness
(micron)
Wet
Dry
150
125
125
Shirish Khare
Sales
7
Quality Code:
Environment :
Severe
Theoretical spreading
rate
(sqm/ltr)
6.4
Application methods
Roller
Brush
Spray
Recommended
Nozzle
Nozzle
orifice
pressure
(X)
X
.017"-.023" 250 bar
X: Recommended (X): Possible
Specification sheet
HEMPEL A/S
Customer:
Project:
Area:
Area size:
1 sqm
System B (Insulated) Stainless steel piping and equipment , operating temperature up to 120C ,Substrate Stainless steel
Remarks:
Normal good painting practice must be followed throughout the entire painting procedure.
Product information:
Shade no.
50630
Volume
solids %
Curing
agent
80
95881
Mixing ratio
volume
3:1
Pot life
Dry to touch
20C
1 h 30 min
20C
3h
Flash
point
C
39
Thinner
08450
Application restrictions
Min. Temp. Max. RH%
C
15
The data, specifications, directions and recommendations (hereinafter "Information") given in this painting specification are based upon test results obtained under controlled or specifically defined conditions and said Information is correct to the
best of our knowledge. The User must satisfy itself that it is appropriate to use the Product in accordance with the Information in the actual conditions under which the Product is intended to be used, and the Manufacturer and Seller do not
guarantee the accuracy, completeness or appropriateness of the Information when the Product is used in those conditions. The provisions regarding Hempels liability in its applicable conditions for sale, delivery and service shall apply to any and
all claims arising out of or in connection with the use of the products recommended above, overleaf or otherwise.
Hempel's PreSale System 2.6.17 (Build 900)
User name:
Printed at:
16.02.2015 11:01 Department name:
Created/Last modified:
16.02.2015 10:40 AESHK0084N Page:
Shirish Khare
Sales
8
Quality Code:
Environment :
Severe
Specification sheet
HEMPEL A/S
Customer:
Project:
Area:
Area size:
1 sqm
System C Carbon steel piping and equipment , operating temperature 120 to 400 C ,Substrate Mild steel
Surface preparation:
Minimum secondary surface preparation mechanical cleaning to St 3 according to ISO
8501-1:2007, apart from cleaning for surface contamination.
Colour
Film thickness
(micron)
Wet
Dry
Shade no.
Treated area
%
Metal grey
Light alu
Total d.f.t.
Hrs=Hour(s)
19840
19000
Mth=Month(s)
150
50
Theoretical spreading
rate
(sqm/ltr)
75
25
100
Application methods
Roller
Brush
Spray
7.2
17.2
Recommended
Nozzle
Nozzle
orifice
pressure
(X)
X
.017"
125 bar
(X)
X
0.017"
125 bar
X: Recommended (X): Possible
N/R=Not Recommended
D.F.T.
Quality no
16900
(micron)
Recoated with
quality no
75
56914
40C
Min.
27 Hrs
30C
Max.
None
Min.
41 Hrs
20C
Max.
None
Min.
55 Hrs
10C
Max.
None
Shirish Khare
Sales
9
Quality Code:
Environment :
Severe
Min.
4 Day
0C
Max.
None
Min.
7 Day
-10C
Max.
None
Min.
15 Day
Max.
None
Specification sheet
HEMPEL A/S
Customer:
Project:
Area:
Area size:
1 sqm
System C Carbon steel piping and equipment , operating temperature 120 to 400 C ,Substrate Mild steel
Remarks:
Normal good painting practice must be followed throughout the entire painting procedure.
1) See product data sheet and / or APPLICATION INSTRUCTIONS regarding drying time and recoating intervals.
Product information:
Shade no.
19840
19000
Volume
solids %
Curing
agent
54
43
Mixing ratio
volume
Pot life
Dry to touch
20C
20C
2h
1h
Flash
point
C
25
30
Thinner
Application restrictions
Min. Temp. Max. RH%
C
08080
08080
The data, specifications, directions and recommendations (hereinafter "Information") given in this painting specification are based upon test results obtained under controlled or specifically defined conditions and said Information is correct to the
best of our knowledge. The User must satisfy itself that it is appropriate to use the Product in accordance with the Information in the actual conditions under which the Product is intended to be used, and the Manufacturer and Seller do not
guarantee the accuracy, completeness or appropriateness of the Information when the Product is used in those conditions. The provisions regarding Hempels liability in its applicable conditions for sale, delivery and service shall apply to any and
all claims arising out of or in connection with the use of the products recommended above, overleaf or otherwise.
Hempel's PreSale System 2.6.17 (Build 900)
User name:
Printed at:
16.02.2015 11:01 Department name:
Created/Last modified:
16.02.2015 10:40 AESHK0084N Page:
Shirish Khare
Sales
10
Quality Code:
Environment :
Severe
Specification sheet
HEMPEL A/S
Customer:
Project:
Area:
Area size:
1 sqm
System F Stainless steel piping and equipment ,operating temperature 120 to 200 C Non insulated. Substrate Stainless steel
Surface preparation:
Oil and grease etc. to be removed by emulsion cleaning. Salts and other contamination to
be removed by high pressure fresh water hosing. Entire area to be roughened to create a
uniform flat finish prior to application of the specified painting system. In severe cases,
abrasive sweep blasting to a uniform flat finish with a dense surface profile may be
necessary. The abrasives used must be non-metallic and metal free. Depending on local
conditions, mechanical cleaning (avoid polishing) may be used.
Colour
Film thickness
(micron)
Wet
Dry
Shade no.
Treated area
%
Light alu
Light alu
Total d.f.t.
Hrs=Hour(s)
19000
19000
Mth=Month(s)
50
50
Theoretical spreading
rate
(sqm/ltr)
25
25
50
Application methods
Roller
Brush
Spray
17.2
17.2
Recommended
Nozzle
Nozzle
orifice
pressure
(X)
X
0.017"
125 bar
(X)
X
0.017"
125 bar
X: Recommended (X): Possible
N/R=Not Recommended
D.F.T.
Quality no
56914
(micron)
Recoated with
quality no
25
56914
40C
Min.
12 Hrs
30C
Max.
None
Min.
18 Hrs
20C
Max.
None
Min.
24 Hrs
10C
Max.
None
Shirish Khare
Sales
11
Quality Code:
Environment :
Severe
Min.
43 Hrs
0C
Max.
None
Min.
72 Hrs
-10C
Max.
None
Min.
6 Day
Max.
None
Specification sheet
HEMPEL A/S
Customer:
Project:
Area:
Area size:
1 sqm
System F Stainless steel piping and equipment ,operating temperature 120 to 200 C Non insulated. Substrate Stainless steel
Remarks:
Normal good painting practice must be followed throughout the entire painting procedure.
Product information:
Shade no.
19000
19000
Volume
solids %
Curing
agent
43
43
Mixing ratio
volume
Pot life
Dry to touch
20C
20C
1h
1h
Flash
point
C
30
30
Thinner
Application restrictions
Min. Temp. Max. RH%
C
08080
08080
The data, specifications, directions and recommendations (hereinafter "Information") given in this painting specification are based upon test results obtained under controlled or specifically defined conditions and said Information is correct to the
best of our knowledge. The User must satisfy itself that it is appropriate to use the Product in accordance with the Information in the actual conditions under which the Product is intended to be used, and the Manufacturer and Seller do not
guarantee the accuracy, completeness or appropriateness of the Information when the Product is used in those conditions. The provisions regarding Hempels liability in its applicable conditions for sale, delivery and service shall apply to any and
all claims arising out of or in connection with the use of the products recommended above, overleaf or otherwise.
Hempel's PreSale System 2.6.17 (Build 900)
User name:
Printed at:
16.02.2015 11:01 Department name:
Created/Last modified:
16.02.2015 10:40 AESHK0084N Page:
Shirish Khare
Sales
12
Quality Code:
Environment :
Severe
Specification sheet
HEMPEL A/S
Customer:
Project:
Area:
Area size:
1 sqm
Systrem I Stainless Steel piping, equipment operating form 200 deg C to 500 Deg C , non insulated
Surface preparation:
Oil and grease etc. to be removed by emulsion cleaning. Salts and other contamination to
be removed by high pressure fresh water hosing. Entire area to be roughened to create a
uniform flat finish prior to application of the specified painting system. In severe cases,
abrasive sweep blasting to a uniform flat finish with a dense surface profile may be
necessary. The abrasives used must be non-metallic and metal free. Depending on local
conditions, mechanical cleaning (avoid polishing) may be used.
Colour
Film thickness
(micron)
Wet
Dry
Shade no.
Treated area
%
Light alu
Light alu
Total d.f.t.
Hrs=Hour(s)
19000
19000
Mth=Month(s)
50
50
Theoretical spreading
rate
(sqm/ltr)
25
25
50
Application methods
Roller
Brush
Spray
17.2
17.2
Recommended
Nozzle
Nozzle
orifice
pressure
(X)
X
0.017"
125 bar
(X)
X
0.017"
125 bar
X: Recommended (X): Possible
N/R=Not Recommended
D.F.T.
Quality no
56914
(micron)
Recoated with
quality no
25
56914
40C
Min.
12 Hrs
30C
Max.
None
Min.
18 Hrs
20C
Max.
None
Min.
24 Hrs
10C
Max.
None
Shirish Khare
Sales
13
Quality Code:
Environment :
Severe
Min.
43 Hrs
0C
Max.
None
Min.
72 Hrs
-10C
Max.
None
Min.
6 Day
Max.
None
Specification sheet
HEMPEL A/S
Customer:
Project:
Area:
Area size:
1 sqm
Systrem I Stainless Steel piping, equipment operating form 200 deg C to 500 Deg C , non insulated
Remarks:
Normal good painting practice must be followed throughout the entire painting procedure.
Product information:
Shade no.
19000
19000
Volume
solids %
Curing
agent
43
43
Mixing ratio
volume
Pot life
Dry to touch
20C
20C
1h
1h
Flash
point
C
30
30
Thinner
Application restrictions
Min. Temp. Max. RH%
C
08080
08080
The data, specifications, directions and recommendations (hereinafter "Information") given in this painting specification are based upon test results obtained under controlled or specifically defined conditions and said Information is correct to the
best of our knowledge. The User must satisfy itself that it is appropriate to use the Product in accordance with the Information in the actual conditions under which the Product is intended to be used, and the Manufacturer and Seller do not
guarantee the accuracy, completeness or appropriateness of the Information when the Product is used in those conditions. The provisions regarding Hempels liability in its applicable conditions for sale, delivery and service shall apply to any and
all claims arising out of or in connection with the use of the products recommended above, overleaf or otherwise.
Hempel's PreSale System 2.6.17 (Build 900)
User name:
Printed at:
16.02.2015 11:01 Department name:
Created/Last modified:
16.02.2015 10:40 AESHK0084N Page:
Shirish Khare
Sales
14
Quality Code:
Environment :
Severe
Specification sheet
HEMPEL A/S
Customer:
Project:
Area:
Area size:
1 sqm
Surface preparation:
Oil and grease etc. to be removed by emulsion cleaning. Entire area to be (high pressure)
fresh water cleaned in order to remove salts and other contaminants. When the surface is
dry: Abrasive blasting to minimum Sa 2 according to ISO 8501-1:2007 with a surface
profile corresponding to Rugotest No. 3 BN 9a.
HEMPADUR 85531
HEMPADUR 85531
Colour
f/c 100
f/c 100
t/u: touch up f/c: full coat s/c: stripe coat
Film thickness
(micron)
Wet
Dry
Shade no.
Treated area
%
Red
Red
Total d.f.t.
Hrs=Hour(s)
50890
50890
Mth=Month(s)
350
350
Theoretical spreading
rate
(sqm/ltr)
300
300
600
Application methods
Roller
Brush
Spray
2.8
2.8
Recommended
Nozzle
Nozzle
orifice
pressure
(X)
X
.021"-.023" 250 bar
(X)
X
.021"-.023" 250 bar
X: Recommended (X): Possible
N/R=Not Recommended
D.F.T.
Quality no
85531
(micron)
Recoated with
quality no
300
85531
40C
Min.
30C
Max.
N/R
N/R
Min.
N/R
20C
Max.
N/R
Min.
N/R
10C
Max.
N/R
Shirish Khare
Sales
15
Quality Code:
Environment :
Immersion
Min.
N/R
0C
Max.
N/R
Min.
N/R
-10C
Max.
N/R
Min.
N/R
Max.
N/R
Specification sheet
HEMPEL A/S
Customer:
Project:
Area:
Area size:
1 sqm
Remarks:
Normal good painting practice must be followed throughout the entire painting procedure.
Product information:
HEMPADUR 85531
HEMPADUR 85531
Shade no.
50890
50890
Volume
solids %
Curing
agent
84
84
97531
97531
Mixing ratio
volume
4:1
4:1
Pot life
Dry to touch
20C
1h
1h
20C
6h
6h
Flash
point
C
14
14
Thinner
08450
08450
Application restrictions
Min. Temp. Max. RH%
C
5
5
The data, specifications, directions and recommendations (hereinafter "Information") given in this painting specification are based upon test results obtained under controlled or specifically defined conditions and said Information is correct to the
best of our knowledge. The User must satisfy itself that it is appropriate to use the Product in accordance with the Information in the actual conditions under which the Product is intended to be used, and the Manufacturer and Seller do not
guarantee the accuracy, completeness or appropriateness of the Information when the Product is used in those conditions. The provisions regarding Hempels liability in its applicable conditions for sale, delivery and service shall apply to any and
all claims arising out of or in connection with the use of the products recommended above, overleaf or otherwise.
Hempel's PreSale System 2.6.17 (Build 900)
User name:
Printed at:
16.02.2015 11:01 Department name:
Created/Last modified:
16.02.2015 10:40 AESHK0084N Page:
Shirish Khare
Sales
16
Quality Code:
Environment :
Immersion
Product Data
HEMPEL'S SILICONE ZINC 16900
Description:
HEMPELS SILICONE ZINC 16900 is a heat resistant zinc pigmented silicone primer. It is air drying at
ambient temperature and resists temperatures up to 400C/750F.
(See REMARKS overleaf)
Recommended use:
As a primer for long-time corrosion protection of steel exposed to high temperatures (from
100C/210F to 400C/750F).
Service temperature:
Maximum service temperature is depending on the subsequent coat. Maximum, dry exposure only:
400C/752F
Certificates/Approvals:
Availability:
PHYSICAL CONSTANTS:
Shade nos/Colours:
Finish:
Volume solids, %:
Theoretical spreading rate:
Flash point:
Specific gravity:
Surface dry:
Dry to touch:
VOC content:
The physical constants stated are nominal data according to the HEMPEL Group's approved formulas.
APPLICATION DETAILS:
Application method:
Thinner (max.vol.):
Nozzle orifice:
Nozzle pressure:
Cleaning of tools:
Indicated film thickness, dry:
Indicated film thickness, wet:
Overcoat interval, min:
Overcoat interval, max:
Safety:
Page: 1/2
Remove oil and grease etc. thoroughly with suitable detergent. Remove salts and other contaminants
by high pressure fresh water cleaning. Abrasive blasting to Sa 2 (ISO 8501-1:2007). If shopprimer is
required, only zinc silicate type is recommended.
APPLICATION CONDITIONS:
Apply only on a dry and clean surface with a temperature above the dew point to avoid condensation.
In confined spaces provide adequate ventilation during application and drying.
PRECEDING COAT:
SUBSEQUENT COAT:
REMARKS:
Note: If used as anticorrosive protection under insulation of high temperature equipment it is very
important that NO moisture can penetrate during slow-down periods. This to avoid risk of "wet
corrosion" when the temperature rises.
Product
1690019840
As supplied
403 g/l
15 vol. % thinning
471 g/l
Weathering/service temperatures: On first exposure to heat the temperature increase from ambient temperature to the required service
temperature must run over a period of 24 hours.
Application(s):
The paint film is somewhat thermoplastic also after heating
Film thicknesses/thinning:
Excessive film thickness must be avoided. THINNER 08080 must be added at application to secure
the low dry film thickness.
For high temperature service, the total dry film thickness of the paint system should preferably be kept
at maximum: 75 micron/3 mils.
Overcoating:
Overcoating intervals related to later conditions of exposure: If the maximum overcoating interval is
exceeded, roughening of the surface is necessary to ensure intercoat adhesion.
Before overcoating after exposure in contaminated environment, clean the surface thoroughly with
high pressure fresh water hosing and allow drying.
A specification supersedes any guideline overcoat intervals indicated in the table.
Environment
Atmospheric, medium
Surface temperature:
HEMPEL'S SILICONE
SERIES
10C (50F)
20C (68F)
30C (86F)
Min
Max
Min
Max
Min
Max
44 h
None
24 h
None
18 h
None
Overcoating note:
Note:
ISSUED BY:
HEMPEL A/S
1690019840
X Move PDS Disclaimer to Second page
This Product Data Sheet supersedes those previously issued.
For explanations, definitions and scope, see Explanatory Notes available on www.hempel.com. Data, specifications, directions and recommendations
given in this data sheet represent only test results or experience obtained under controlled or specially defined circumstances. Their accuracy,
completeness or appropriateness under the actual conditions of any intended use of the Products herein must be determined exclusively by the Buyer
and/or User.
The Products are supplied and all technical assistance is given subject to HEMPEL's GENERAL CONDITIONS OF SALES, DELIVERY AND SERVICE, unless
otherwise expressly agreed in writing. The Manufacturer and Seller disclaim, and Buyer and/or User waive all claims involving, any liability, including but
not limited to negligence, except as expressed in said GENERAL CONDITIONS for all results, injury or direct or consequential losses or damages arising
from the use of the Products as recommended above, on the overleaf or otherwise. Product data are subject to change without notice and become void
five years from the date of issue.
Page: 2/2
Product Data
HEMPADUR MASTIC 45881
High temperatures 45881: BASE 45889: CURING AGENT 95881
Description:
HEMPADUR MASTIC 45881 is a two-component polyamide adduct cured, high solids, high build
epoxy paint. It forms a hard and tough coating, has good wetting properties.
Recommended use:
As a selfprimed, surface tolerant paint system or as an intermediate or finishing coat in heavy duty
paint systems where low VOC and high film build are required.
Multipurpose coating as per specification for maintenance and minor repairs in immersed areas
including ballast tanks and underwater hull specifically in those cases where a need for few products
outweighs more specialised coatings.
Can be specified where extended recoating properties for polyurethane topcoats are requested
(typically travel coating). May be used directly on cured zinc silicate (GALVOSIL products) or spraymetallized surfaces to minimize popping.
Service temperature:
Certificates/Approvals:
In accordance with Aramcos specification APCS 1, APCS 12, APCS 26 and 26T.
Tested for non-contamination of grain cargo at the Newcastle Occupational Health & Hygiene, Great
Britain.
Approved as a low flame spread material when used as part of a predefined paint system. Please refer
to Declaration of Conformity on www.Hempel.com for further details.
Complies with EU Directive 2004/42/EC: subcategory j.
Availability:
PHYSICAL CONSTANTS:
Shade nos/Colours:
Finish:
Volume solids, %:
Theoretical spreading rate:
Flash point:
Specific gravity:
Dry to touch:
Fully cured:
VOC content:
12170* / Grey.
Semi-gloss
80 1
6.4 m2/l [256.6 sq.ft./US gallon] - 125 micron/5 mils
35 C [95 F]
1.5 kg/litre [12.1 lbs/US gallon]
3 hour(s) 30C/86F
5 day(s) 30C/86F
218 g/l [1.8 lbs/US gallon]
APPLICATION DETAILS:
Version, mixed product:
Mixing ratio:
Application method:
Thinner (max.vol.):
Pot life (Airless spray):
Pot life (Brush):
Nozzle orifice:
Nozzle pressure:
Cleaning of tools:
Indicated film thickness, dry:
Indicated film thickness, wet:
Overcoat interval, min:
Overcoat interval, max:
Safety:
45881
BASE 45889: CURING AGENT 95881
3 : 1 by volume
Airless spray / Brush
< 5% HEMPEL'S THINNER 08450, depending on purpose (see REMARKS overleaf)
1.5 hour(s) 30C/86F
2 hour(s) 30C/86F
0.017 - 0.023 " According to separate APPLICATION INSTRUCTIONS
250 bar [3625 psi]
HEMPEL'S TOOL CLEANER 99610
125 micron [5 mils] see REMARKS overleaf
150 micron [6 mils]
see REMARKS overleaf
see REMARKS overleaf
Handle with care. Before and during use, observe all safety labels on packaging and paint containers,
consult HEMPEL Safety Data Sheets and follow all local or national safety regulations.
Page: 1/3
New steel: Abrasive blasting to minimum Sa 2 (ISO 8501-1:2007) with a surface profile
corresponding to Rugotest No. 3, N9a to N10, preferably BN9a to BN10, Keane-Tator Comparator, 2.0
G/S or ISO Comparator, Medium (G).
Zinc silicate painted or spray-metallized surfaces: Remove oil and grease, etc. with suitable
detergent. Remove salt and other contaminants by (high pressure) fresh water cleaning. Zinc salts
(white rust) must be removed by high pressure hosing combined with rubbing with a stiff nylon brush if
necessary. It is recommended to recoat spray-metallized surfaces as soon as possible to avoid
possible contamination.
Concrete: Remove slip agent and other possible contaminants by emulsion washing followed by high
pressure hosing with fresh water. Remove scum layer and loose matter to a hard, rough and uniform
surface, preferably by abrasive blasting, possibly by other mechanical treatment or acid etching. Seal
surface with suitable sealer, as per relevant painting specification.
Repair and maintenance: Remove oil and grease etc. thoroughly with suitable detergent. Remove
salts and other contaminants by high pressure fresh water cleaning. Clean damaged areas thoroughly
by power tool cleaning to minimum St 2 (spot-repairs) or by abrasive blasting to min. Sa 2, preferably
to Sa 2 (ISO 8501-1:1988). Improved surface preparation will improve the performance of the
product. As an alternative to dry cleaning, water jetting to sound, well adhering coat and/or to steel.
Intact coat must appear with roughened surface after the water jetting. By water jetting to steel,
cleanliness shall be: Wa 2 -Wa 2 (atmospheric exposure) / minimum Wa 2 (immersion) (ISO
8501-4:2006). Feather edges to sound and intact areas. Dust off residues. Touch up to full film
thickness. On pit-corroded surfaces, excessive amounts of salt residues may call for high pressure
water jetting, wet abrasive blasting or, alternatively, dry abrasive blasting, high pressure fresh water
hosting, drying, and finally dry abrasive blasting again.
APPLICATION CONDITIONS:
Apply only on a dry and clean surface with a temperature above the dew point to avoid condensation.
Use only where application and curing can proceed at temperatures above: 15C/59F.
The temperature of paint itself should be 15C/59F or above. In confined spaces provide adequate
ventilation during application and drying.
PRECEDING COAT:
SUBSEQUENT COAT:
REMARKS:
Product
4588112170
As supplied
218 g/l
5 vol. % thinning
250 g/l
Weathering/service temperatures: The natural tendency of epoxy coatings to chalk in outdoor exposure and to become more sensitive to
mechanical damage and chemical exposure at elevated temperatures is also reflected in this product.
Application(s):
Application onto zinc silicate or spray-metallized surfaces (thinning): It is recommended to apply the
paint by using a "mist-coat" procedure provided the paint temperature is approximately above:
20C/68F. A thin, undiluted coat is applied (the mist coat) and after a few minutes, a second coat is
applied in the full specified film thickness. If the paint temperature is below: 20C/68F, thinning (max
15%) may be required.
Film thicknesses/thinning:
May be specified in another film thickness than indicated depending on purpose and area of use. This
will alter spreading rate and may influence drying time and overcoating interval. Normal range dry is:
125-200 micron/5-8 mils. May be specified in lower film thickness for which purpose additional thinning
is required, please see separate APPLICATION INSTRUCTIONS. Avoid application of excessive
film thicknesses.
Shades:
The product is also available in a Micaceous Iron Oxide (MIO) pigmented shade (Shade no. 12430
reddish grey ) and in aluminium pigmented shades (Shade nos. 19870 - dark alu and 19000 - light alu).
Overcoating:
Overcoating intervals related to later conditions of exposure: If the maximum overcoating interval is
exceeded, roughening of the surface is necessary to ensure intercoat adhesion.
Before overcoating after exposure in contaminated environment, clean the surface thoroughly with
high pressure fresh water hosing and allow drying.
A specification supersedes any guideline overcoat intervals indicated in the table.
Environment
Atmospheric, medium
Surface temperature:
20C (68F)
Min
Max
Min
Max
Min
Max
7h
Ext.
6h
Ext.
4h
Ext.
HEMPATEX
7h
12 h
6h
9h
4h
6h
HEMPATHANE
7h
Ext.
6h
Ext.
4h
Ext.
12 h
30 d
10 h
7h
15 d
HEMPADUR
40C (104F)
HEMPADUR
Environment
30C (86F)
Immersion
Page: 2/3
23 d
Note:
ISSUED BY:
HEMPEL A/S
4588112170
X Move PDS Disclaimer to Second page
This Product Data Sheet supersedes those previously issued.
For explanations, definitions and scope, see Explanatory Notes available on www.hempel.com. Data, specifications, directions and recommendations
given in this data sheet represent only test results or experience obtained under controlled or specially defined circumstances. Their accuracy,
completeness or appropriateness under the actual conditions of any intended use of the Products herein must be determined exclusively by the Buyer
and/or User.
The Products are supplied and all technical assistance is given subject to HEMPEL's GENERAL CONDITIONS OF SALES, DELIVERY AND SERVICE, unless
otherwise expressly agreed in writing. The Manufacturer and Seller disclaim, and Buyer and/or User waive all claims involving, any liability, including but
not limited to negligence, except as expressed in said GENERAL CONDITIONS for all results, injury or direct or consequential losses or damages arising
from the use of the Products as recommended above, on the overleaf or otherwise. Product data are subject to change without notice and become void
five years from the date of issue.
Page: 3/3
Product Data
HEMPATHANE HS 55610
55610: BASE 55619: CURING AGENT 97050
Description:
Recommended use:
As a VOC-compliant, high-build finishing coat for protection of structural steel in corrosive environment.
May be specified as a one coat "Direct To Metal" system in environments classified as C2 and C3.
Service temperature:
Certificates/Approvals:
Approved as a low flame spread material when used as part of a predefined paint system. Please refer
to Declaration of Conformity on www.Hempel.com for further details.
Availability:
PHYSICAL CONSTANTS:
Shade nos/Colours:
Finish:
Volume solids, %:
Theoretical spreading rate:
Flash point:
Specific gravity:
Surface dry:
Dry to touch:
Fully cured:
VOC content:
APPLICATION DETAILS:
Version, mixed product:
Mixing ratio:
Application method:
Thinner (max.vol.):
Pot life:
Nozzle orifice:
Nozzle pressure:
Cleaning of tools:
Indicated film thickness, dry:
Indicated film thickness, wet:
Overcoat interval, min:
Overcoat interval, max:
Safety:
55610
BASE 55619: CURING AGENT 97050
7:1 by volume
Airless spray (see REMARKS overleaf) / Brush (see REMARKS overleaf)
08080 (5%) / 08080 (5%)
2 hour(s) 20C/68F
0.017 to 0.021 "
175 bar [2537.5 psi]
(Airless spray data are indicative and subject to adjustment)
HEMPEL'S THINNER 08080
100 micron [4 mils] / 4 mils (see REMARKS overleaf)
150 micron [6 mils] / 6 mils
see REMARKS overleaf
see REMARKS overleaf
Handle with care. Before and during use, observe all safety labels on packaging and paint containers,
consult HEMPEL Safety Data Sheets and follow all local or national safety regulations.
Page: 1/2
HEMPATHANE HS 55610
SURFACE PREPARATION:
According to specification.
APPLICATION CONDITIONS:
Apply only on a dry and clean surface with a temperature above the dew point to avoid condensation.
Minimum temperature for curing is: -10C/14F
At the freezing point and below be aware of the risk of ice on the surface, which will hinder adhesion.
The film formation may be adversely affected by light rain, high humidity and/or condensation during
application and the following interval after application:24 hours , 20C/68F
In confined spaces provide adequate ventilation during application and drying.
PRECEDING COAT:
According to specification. Recommended systems are: HEMPADUR FAST DRY 15560, HEMPADUR
MASTIC 45880/45881
SUBSEQUENT COAT:
None.
REMARKS:
VOC - EU Directive 2004/42/EC:
Product
5561010000
Not available.
As supplied
337 g/l
5 vol. % thinning
363 g/l
Colours/Colour stability:
Certain lead-free red and yellow colours may discolour when exposed to chlorine-containing
atmosphere. To obtain full opacity, an extra coat may be necessary, especially for certain lead-free
colours in red, orange, yellow and green.
Weathering/service temperatures: At service temperature above 100C/212F, slight discolouration may be expected. The product will
become softer.
Application(s):
When specified as a one coat Direct to Metal-system follow Good Painting Practise and apply
stripe coating before the spray application on areas difficult to cover properly by spray application.
CURING AGENT 97050 : is sensitive to moisture.
Even small traces of water in the mixed paint will reduce the pot life and result in film defects.
Film thicknesses/thinning:
May be specified in another film thickness than indicated depending on purpose and area of use. This
will alter spreading rate and may influence drying time and overcoating interval. Normal range dry is:
minimum 50 micron/2 mils (diluted), minimum 75 micron/3 mils (undiluted), maximum 125 micron/5
mils
Storage Conditions:
Store in a dry place and keep the can tightly closed until use.
Shades:
This product is available in several aluminium pigmented shades with different volume solids content.
Contact HEMPEL for more information.
Curing agent:
Open curing agent cans with caution as overpressure might exist.
Overcoating:
Overcoating intervals related to later conditions of exposure: If the maximum overcoating interval is
exceeded, roughening of the surface is necessary to ensure intercoat adhesion.
Before overcoating after exposure in contaminated environment, clean the surface thoroughly with
high pressure fresh water hosing and allow drying.
A specification supersedes any guideline overcoat intervals indicated in the table.
Environment
Atmospheric, medium
Surface temperature:
HEMPATHANE
-10C (14F)
0C (32F)
20C (68F)
Min
Max
Min
Max
Min
Max
18 h
None
9h
None
6h
None
Overcoating note:
Note:
A completely clean surface is mandatory to ensure intercoat adhesion, especially at long overcoating
intervals. Any dirt, oil, grease, and other foreign matter must be removed with suitable detergent
followed by (high pressure) fresh water cleaning. Salts to be removed by fresh water hosing.
To check whether the quality of the surface cleaning is adequate, a test patch may be relevant.
HEMPATHANE HS 55610 For professional use only.
ISSUED BY:
HEMPEL A/S
5561010000
X Move PDS Disclaimer to Second page
This Product Data Sheet supersedes those previously issued.
For explanations, definitions and scope, see Explanatory Notes available on www.hempel.com. Data, specifications, directions and recommendations
given in this data sheet represent only test results or experience obtained under controlled or specially defined circumstances. Their accuracy,
completeness or appropriateness under the actual conditions of any intended use of the Products herein must be determined exclusively by the Buyer
and/or User.
The Products are supplied and all technical assistance is given subject to HEMPEL's GENERAL CONDITIONS OF SALES, DELIVERY AND SERVICE, unless
otherwise expressly agreed in writing. The Manufacturer and Seller disclaim, and Buyer and/or User waive all claims involving, any liability, including but
not limited to negligence, except as expressed in said GENERAL CONDITIONS for all results, injury or direct or consequential losses or damages arising
from the use of the Products as recommended above, on the overleaf or otherwise. Product data are subject to change without notice and become void
five years from the date of issue.
Page: 2/2
Product Data
HEMPEL'S SILICONE ALUMINIUM 56914
Description:
HEMPEL'S SILICONE ALUMINIUM 56914 is a heat resistant aluminium pigmented polysiloxane paint
which cures to a hard film at ambient conditions.
Recommended use:
For long-term protection of hot pipelines, exhaust pipes, smoke stacks and other hot surfaces. In
corrosive environment see PRECEDING COAT overleaf.
Service temperature:
Certificates/Approvals:
Availability:
PHYSICAL CONSTANTS:
Shade nos/Colours:
Finish:
Volume solids, %:
Theoretical spreading rate:
Flash point:
Specific gravity:
Surface dry:
Dry to touch:
VOC content:
Shelf life:
19000/ Aluminium
Semi-flat see REMARKS overleaf
43 1
17.2 m2/l [689.7 sq.ft./US gallon] - 25 micron/1 mils
28 C [82.4 F]
1.2 kg/litre [9.7 lbs/US gallon]
1 approx. hour(s) 20C/68F
2 hour(s) 20C/68F
465 g/l [3.9 lbs/US gallon]
1 year (25C/77F) from time of production. Depending on storage conditions, mechanical stirring may
be necessary before usage.
The physical constants stated are nominal data according to the HEMPEL Group's approved formulas.
APPLICATION DETAILS:
Application method:
Thinner (max.vol.):
Nozzle orifice:
Nozzle pressure:
Cleaning of tools:
Indicated film thickness, dry:
Indicated film thickness, wet:
Overcoat interval, min:
Overcoat interval, max:
Safety:
Page: 1/2
Remove oil and grease etc. thoroughly with suitable detergent. Remove salts and other contaminants
by high pressure fresh water cleaning. Abrasive blasting to Sa 2 (ISO 8501-1:2007).
APPLICATION CONDITIONS:
Apply only on a dry and clean surface with a temperature above the dew point to avoid condensation.
Minimum relative humidity: 50% . In confined spaces provide adequate ventilation during application
and drying.
PRECEDING COAT:
SUBSEQUENT COAT:
None.
REMARKS:
VOC - EU Directive 2004/42/EC:
Not available.
Product
5691419000
As supplied
465 g/l
5 vol. % thinning
484 g/l
Colours/Colour stability:
After exposure to heat the gloss is reduced.
Weathering/service temperatures: On first exposure to heat the temperature increase from ambient temperature to the required service
temperature must run over a period of 24 hours.
Application(s):
The coating will be fully cured after: 7 days , 20C/68F
When the paint is applied on zinc silicate coatings, popping may occur after application or after first
heating up. To avoid popping it is recommended to follow the procedure: A thin, undiluted coat is
applied (the mist coat) and after a few minutes, a second coat is applied in the full specified film
thickness
Film thicknesses/thinning:
May be specified in another film thickness than indicated depending on purpose and area of use. This
will alter spreading rate and may influence drying time and overcoating interval. Normal range dry is:
20-40 micron/0.8-1.6 mils. Excessive film thickness must be avoided. THINNER 08080 can be added
at application to secure the low dry film thickness.
For high temperature service, the total dry film thickness of the paint system should preferably be kept
at maximum: 75 micron/3 mils.
Overcoating note:
May be overcoated when through dry: 24 hours 20C/68F
Before overcoating after exposure in contaminated environment, clean the surface thoroughly with
high pressure fresh water hosing and allow drying.
Note:
HEMPEL'S SILICONE ALUMINIUM 56914 For professional use only.
ISSUED BY:
HEMPEL A/S
5691419000
Page: 2/2
Product Data
HEMPADUR 85531
85531 : BASE 85539 : CURING AGENT 97531
Description:
HEMPADUR 85531 is an amine-adduct, cured epoxy coating. It is a hard, impact and abrasion resistant
coating eg for exterior pipelines. The material has excellent properties in respect of temperature
resistance, mechanical and chemical resistance and cathodic disbondment resistance.
Recommended use:
For new constructions as well as field-applied renovation and repair coating. As a self-primed, high
build coating primarily for protection of interior of steel pipes and of exterior of steel pipes in severely
corrosive environment, including permanent immersion.
HEMPADUR 85531 is an excellent material for repair and can be applied to lines while in service
temperature up to 90C/194F.
Service temperature:
Availability:
PHYSICAL CONSTANTS:
Shade nos/Colours:
Finish:
Volume solids, %:
Theoretical spreading rate:
Flash point:
Specific gravity:
Surface dry:
Dry to touch:
Fully cured:
VOC content:
50890 / Red.
glossy
84 1
2.4 m2/l [96.2 sq.ft./US gallon] - 350 micron/14 mils
14 C [57.2 F]
1.7 kg/litre [13.9 lbs/US gallon]
2 hour(s) 20C/68F
6 hour(s) 20C/68F
7 day(s) 20C/68F
167 g/l [1.4 lbs/US gallon]
The physical constants stated are nominal data according to the HEMPEL Group's approved formulas.
APPLICATION DETAILS:
Version; mixed product:
Mixing ratio:
Application method:
Thinner (max.vol.):
Pot life:
Nozzle orifice:
Nozzle pressure:
Cleaning of tools:
Indicated film thickness, dry:
Indicated film thickness, wet:
Recoat interval, min:
Recoat interval, max:
Safety:
85531
BASE 85539 : CURING AGENT 97531
4 : 1 By volume
Airless spray
08450 (5%)
1 hour(s) 20C/68F
0.021 - 0.023 "
250 [3625 psi]
(Airless spray data are indicative and subject to adjustment)
HEMPEL'S TOOL CLEANER 99610
350 micron [14 mils]
425 micron [17 mils]
According to specification.
According to specification.
Handle with care. Before and during use, observe all safety labels on packaging and paint containers,
consult HEMPEL Safety Data Sheets and follow all local or national safety regulations.
Page: 1/2
HEMPADUR 85531
SURFACE PREPARATION:
New steel: Remove oil and grease etc. thoroughly with suitable detergent. Remove salts and other
contaminants by high pressure fresh water cleaning. Gritblasting to minimum Sa 2 (ISO 8501-1:1988)
with a surface profile equivalent tu Rugotest No. 3 BN10a, Keane-Tator Comparator, min. 3.0 G/S, or
ISO Comparator rough MEDIUM (G). After blasting, clean the surface carefully from abrasives and
dust.
Repair and maintenance: Remove oil and grease etc. thoroughly with suitable detergent. Remove
salts and other contaminants by high pressure fresh water cleaning. Gritblasting to minimum Sa 2
(ISO 8501-1:1988) with a surface profile equivalent tu Rugotest No. 3 BN10a, Keane-Tator
Comparator, min. 3.0 G/S, or ISO Comparator rough MEDIUM (G). After blasting, clean the surface
carefully from abrasives and dust.
APPLICATION CONDITIONS:
Apply only on a dry and clean surface with a temperature above the dew point to avoid condensation. In
confined spaces provide adequate ventilation during application and drying. Use only where application
and curing can proceed at temperatures above: 5C/41F The temperature of the paint itself should be
above: 15C/59F The best result is obtained at: 20-30C/68-86F
PRECEDING COAT
None.
SUBSEQUENT COAT:
REMARKS:
Recoating intervals:
Nota:
ISSUED BY:
The indicated recoat intervals will normally only apply in connection with touch-up of too low dry film
thicknesses.
If the maximum recoating interval is exceeded, roughening of the surface is necessary to ensure
intercoat adhesion.
HEMPADUR 85531 For professional use only.
HEMPEL A/S
8553150890
Page: 2/2
Surface preparation:
Note:
Another risk is remains of a hard black rust scale being cleaned to an apparent brightness
without showing any adhesive defects.
Page 1 of 5
HEMPADUR MASTIC 45880/45881 being a high solids and a relatively high viscosity
material, may require special measures to be taken at application.
Recommended airless spray equipment:
Pump ratio:
Pump output:
min. 45:1
12 litres/minute (theoretical)
Input pressure:
Spray hoses:
Regular surfaces:
After finishing the application, clean the equipment immediately with THINNER 08450 or
HEMPELS TOOL CLEANER 99610.
Note: Increasing hose diameter may increase paint flow, thereby improving the spray fan. If
longer hoses are necessary it may be necessary to raise the pump ratio to 60:1,
maintaining the high output capacity of the pump.
Alternatively up to approx. 5% THINNER 08450 may be added, but thinning must be done
with care as the anti-sagging properties are drastically reduced by overthinning.
Airless spray data are indicative and subject to adjustment.
Induction time:
Spray application:
Page 2 of 5
At application with hand tools, brush, but especially by roller the natural tendency to a more
uneven paint film obtained by these methods, is to be counteracted by more coats applied.
If at all possible each coat is to be applied across the preceding one - in general follow good
painting practise.
On poorly prepared surfaces it is always recommended to apply the first coat by brush.
Extra thinning will facilitate the penetration of the paint material, but will also require an
extra layer to be applied.
Please note that the thixotropic nature of HEMPADUR MASTIC 45880/45881 may give a
rather "wavy" surface of the paint just after application. This smoothens at drying, but can
make it necessary to let the wet film readings be of a higher value than indicated. In many
cases the wet film thickness, reading should be 25-50 micron/1-2 mils higher than
calculated. As the wavy surface becomes more smooth during drying these extra wet film
thickness readings will not cause a higher paint consumption than otherwise stipulated.
Film thickness/thinning:
Pot life:
When measured under standard conditions the pot life is 1 hour at 20C/68F for
HEMPADUR MASTIC 45880 respectively 1 hours at 30C/86F for HEMPADUR MASTIC
45881. However, for a 20 litres/5 US gallons mix, and used under warm climate
conditions, the heat developed by the chemical reaction between BASE and CURING AGENT
may make the corresponding practical pot life shorter.
Therefore: At high temperatures, use the paint immediately after mixing irrespective of
equipment.
Physical data
versus temperature:
Drying time and overcoating interval vary with film thickness, temperature and later
exposure conditions:
HEMPADUR MASTIC 45880 in a dry film thickness of 125 micron/5 mils:
Surface temperature:
-5C/23F
0C/32F
10C/50F
20C/68F
30C/86F
40C/104F
3 days
2,5 months
36 hours
1 month
12 hours
14 days
4 hours
7 days
3 hours
5 days
2 hours
3 days
10C/50F
20C/68F
30C/86F
40C/104F
21 hours
30 hours
36 hours
7 hours
10 hours
12 hours
5 hours
8 hours
9 hours
4 hours
6 hours
7 hours
-5C/23F
0C/32F
Atmospheric, medium
5 days
63 hours
Atmospheric, severe
7 days
3,5 days
Immersion1
8,5 days
4,5 days
1. Not relevant for HEMPATHANE qualities
Page 3 of 5
-5C/23F
0C/32F
10C/50F
20C/68F
30C/86F
40C/104F
Extended*
Extended*
1 months
Extended*
Extended*
23 days
Extended*
Extended*
15 days
Atmospheric, medium
Extended*
Extended*
Extended*
Extended*
Extended*
Atmospheric, severe
52 days
27 days
9 days
3 days
54 hours
* Depending on actual local conditions, extended maximum overcoating intervals may apply.
Please contact Hempel for further advice.
Extended*
40 hours
Extended*
Extended*
3 months
Extended*
Extended*
3 months
Extended*
Extended*
2 months
Notes:
Avoid sudden drops in (substrate) temperatures during drying/initial curing.
20C/68F
4 hours
7 days
30C/86F 40C/104F
3 hours
5 days
2 hours
3 days
7 hours
10 hours
12 hours
6 hours
8 hours
10 hours
4 hours
6 hours
7 hours
20C/68F
30C/86F 40C/104F
Extended*
Extended*
1 months
Extended*
Extended*
23 days
Extended*
Extended*
15 days
Extended*
3 days
Extended*
54 hours
Extended*
36 hours
Page 4 of 5
Handle with care. Before and during use, observe all safety labels on packaging and paint
containers, consult HEMPEL Material Safety Data Sheets and follow all local or national
safety regulations. Avoid inhalation, avoid contact with skin and eyes, and do not swallow.
Take precautions against possible risks of fire or explosions as well as protection of the
environment. Apply only in well ventilated areas.
ISSUED BY:
Page 5 of 5