Adding Water to Concrete on the Jobsite


The addition of water to concrete on the jobsite is still one of the biggest problems facing the ready-
mix concrete industry today. Concrete is one of the few building materials whose quality and
performance characteristics can be imperiled after the product is transported from the manufacturing
facility.

How to Address Issues with Water and Concrete Integrity


On many jobsites, the addition of water is at the discretion of the finishers, whose concerns for in-place
concrete durability and strength are often swept aside in favor of ease and speed of placement. So, is it OK
to add water to concrete on the jobsite? And, if so, are there any guidelines or specifications that might help
the industry protect itself from product liability problems and unjust replacement costs?

Fortunately, ASTM C94, "Standard Specification for Ready-Mixed Concrete," addresses these problems in
detail. Unless otherwise specified, water can be added, one time only, to bring the slump of that particular
load within the range specified for the project. But the addition of water cannot increase the water-cement
ratio above the maximum permitted by the mix design. This presupposes that the person responsible for
adjusting the slump knows how much more water can be added to the truck before the proper water-cement
ratio is exceeded. Many ready-mix concrete producers are solving this problem by printing the necessary
information on the delivery tickets, easily done at plants using computerized batching.

If all the water allowed by the approved mix design has already been added and the slump is still below the
requirement, the accepting authority has the option of adding more water at his own risk or rejecting the
load.

Slump Tolerances
It is impossible to bring concrete exactly to a specified slump on a consistent basis. ASTM C94 has provided
some suggested tolerances that should be followed if the project specifications do not mention any.
If the specifications for slump are written as a target requirement, not a "maximum" or "not to exceed"
requirement, the tolerances are as follows:

Tolerances for Nominal Slumps


Specified Target Tolerance
2 inches and less ±0.5 inch
Greater than 2 inches and less than or equal to 4 inches ±1.0 inch
More than 4 inches ±1.5 inches

When the project specifications for slump are written as a "maximum" or "not to exceed" requirement, the
tolerances are as follows:

Specified Slump
If 3 inches or less If more than 3 inches
Plus tolerance 0 0
Minus tolerance 1.5" 2.5"

Jobsite Delays
One major problem encountered by concrete producers occurs when a mixer truck is delayed on the jobsite.
Although it might have been within the specified range of slump when the truck arrived, hot temperatures
can cause the concrete to lose enough workability that the specified slump can only be reached by
exceeding the water-cement ratio. ASTM C94 covers this eventuality, too. It states that, "Concrete shall be
available within the permissible range of slump for a period of 30 minutes starting either on arrival at the
jobsite or after the initial slump adjustment, whichever is later." It further states, "If the user is unprepared for
discharge of the concrete from the vehicle, the producer shall not be responsible for the limitation of
minimum slump after 30 minutes have elapsed starting either on arrival of the vehicle at the prescribed
destination or at the requested delivery time, whichever is later."

In other words, once the truck arrives at the jobsite, and assuming it isn't early, the driver is responsible for
keeping the slump within the permissible range for about 30 minutes. If it takes longer than that to discharge
the load, and more water is needed to maintain the slump, that water is the responsibility of the user.

For further protection of the concrete producer, ASTM C94 also imposes a limit on the amount of time the
concrete can remain on the truck. The user must have discharged all the concrete from the truck within 90
minutes of batch time. This limit can be extended, at the discretion of the contractor, if the concrete is
workable enough to permit placement without the further addition of water.

http://www.lafarge-na.com/wps/portal/na/en/3_A_11_11-Adding_Water_to_Concrete_on_the_Jobsite?print=yes 1/2
2/1/2018 Adding Water to Concrete on the Jobsite < Concrete < Aggregates & Concrete: Lafarge: Print
Lafarge North America is committed to providing the best possible service to our customers. For more
information about concrete or concrete materials, please contact your Lafarge sales representative or